English

Vacuum Investment Casting a Combustor Casing in Hastelloy X

Table of Contents
Why route a combustor casing through vacuum investment casting?
Wax injection holds ±0.10 mm on a 193 mm casing
How do shell and pour keep a 2.5 mm wall filled?
Solution treatment at 1180 °C opens the cutting window
Where does CNC stop and inspection start?
Two 3D scans bracket 1.0 mm of stock removal
FAQs

A 2.5 mm combustor casing wall fills only while the shell holds 900 °C and the chamber holds 5 Pa. Vacuum investment casting a combustor casing in Hastelloy X fixes those numbers first, then runs the wax pattern, the shell layers and the pour as one sequence. The work stops at an as-cast blank with 1.0 mm of stock on the flange faces; heat treatment, two scans and cutting come after.

Oblique view of a conical casing with two end flanges and a side boss

Top view of the eight-hole flange with a boss inside the bore

Why route a combustor casing through vacuum investment casting?

This combustor casing goes through vacuum investment casting because a sand mold cannot hold a 2.5 mm conical wall, and one part does not pay for a permanent die. A sand route needs about 3 mm of section before draft is added, so the wall would be thickened, cast and then cut back from outside. The wax pattern carries the geometry instead, and its die is the only hard tool the route needs.

The die follows the model plus stock, so the tool holds the geometry rather than a minimum section. A billet route reaches the outer cone but not the inner one, where the ⌀61.5 +0.3/+0.1 spigot and the ⌀24 +0.4/0 boss sit. Open ends at both faces also let the shell be built and the metal reach the wall without a ceramic core.

The route is the right one while three conditions hold:

  • The wall runs 1.5 mm to 3 mm, below the section a sand mold can fill.

  • One part or a small batch is needed, so the wax die is the only tool that has to be cut.

  • Assembly faces are machined afterwards, and the blank can carry 1.0 mm of stock.

All three hold on this 193 mm casing; when one fails, the route changes before the first pattern is molded. The forming half of the chain ends at the blank, and the dimensional half starts at the furnace door; one vacuum investment casting plan for a combustor casing covers both.

Batch size decides the tool count, not the process. One casting needs a wax die and a shell; a hundred castings need the same wax die and a longer run of shells, so the die is cut once either way.

Wax injection holds ±0.10 mm on a 193 mm casing

Wax injection holds ±0.10 mm across the full 193 mm height, so the 2.5 mm wall reaches the shell already in place. The die is cut to the model plus 1.0 mm on the machined faces, and the pattern leaves the die as one piece. A pattern assembled from pieces carries a seam ridge that the shell copies.

Pattern wax is injected at 58 °C and 0.3 MPa, then held for 30 s before the die opens. The hold is what stops the wall from pulling back where the section changes, and a short hold shows up first at the flange. Change the hold and the wall moves before the pattern is out of the die.

±0.10 mm over 193 mm is about 0.05 % of the part, and every later step inherits that band. The band sits inside the 1.0 mm face stock, so pattern error is absorbed before the first cut. It does not absorb a wrong wall: on a 2.5 mm section a 0.2 mm pattern error is 8 % of the thickness.

The first pattern off a new die is measured and sectioned before a tree is built. A die correction at that point takes a day; the same correction after the first casting takes a cycle.

Each pattern is checked for chipped corners and flash at the bench, and a pattern that fails does not go to the tree. The pattern also carries the casting gate stubs, so the two casting gates on the cone are molded rather than cut later. That keeps each casting gate in the same place from pattern to pattern, which is what makes the pour window usable.

How do shell and pour keep a 2.5 mm wall filled?

Shell preheat and pour temperature keep the 2.5 mm wall filled, and neither one works alone. At a 900 °C shell the metal front stays liquid long enough to cross mid-cone; against a cold shell it stops and a cold shut forms.

Shell build runs two corundum face coats over three semi-mullite backup coats. Layer drying takes 8 h at 22 °C and 50 % relative humidity, and that drying is where the calendar time goes. Dewax runs at 0.6 MPa for 8 min, and the burnout at 900 °C for 2 h doubles as the shell preheat.

The face layers do the surface work and the backup layers hold the shape. A shell that is too thin loses heat out of the face before the front arrives, and one that is too thick cracks when the pour lands.

The melt is Hastelloy X (UNS N06002) in a 50 kg vacuum induction furnace, held at 5 Pa or lower, refined at 1450 °C for 5 min and poured at 1420 ± 10 °C. Pouring at that pressure and shell temperature leaves the gas in the chamber rather than in the wall. That window belongs to this grade; Hastelloy alloy vacuum investment casting is where the alloy-specific limits sit.

A cold shut forms where the front stops moving, and on a 193 mm cone that point sits mid-wall. Two casting gates on the cone keep the front moving past it. In-mold cooling for 60 min holds the part still while the last section feeds.

The window the foundry holds from the first pattern to the last casting is set out below.

Stage

Setting

Unit

Wax injection

58

°C

Injection pressure

0.3

MPa

Shell burnout

900

°C

Melt temperature

1450

°C

Pour temperature

1420 ± 10

°C

Chamber vacuum

5 or lower

Pa

In-mold cooling

60

min

Outside that window, a 2.5 mm section either fails to fill or carries shrinkage porosity into the flange transition. Neither shows on the surface, which is why the blank is radiographed before it is cut.

Solution treatment at 1180 °C opens the cutting window

Solution treatment at 1180 °C dissolves the cast carbide network and leaves the casing cuttable at a steady hardness. Cast structure left in place makes the cut unpredictable: hardness varies across the wall and the tool load follows it.

The sequence after the shell comes off has four steps, and none of them can move:

  1. Enter the furnace within 24 h of cutting the shell off.

  2. Solution treat at 1180 °C for 1 h, then cool at 2 bar argon.

  3. Stress relieve at 850 °C for 2 h with the furnace cooling.

  4. Re-measure the datum within 24 h of the furnace door opening.

Those four steps hold the hardness near 90 HRB and keep the movement after quenching measurable rather than random. A skip in the chain does not show up as a defect; it shows up as a dimension that will not repeat.

The heat-treated flange is accepted at 0.30 mm flatness, and the machined target is 0.05 mm. The difference between those two numbers is stock for the cut, not a tolerance the foundry chases.

Cooling from 1180 °C moves a 2.5 mm wall and a thick flange at different rates, so the flange bows while the cone stays round. Clamping through the cool-down and staging the argon pressure narrows that movement. The part is measured after it is released and before it is cut.

A superalloy heat treatment cycle at these settings, solution treatment first and stress relief second, is what opens the computer numerical control (CNC) cut that follows. Cut a bowed blank and the flatness has to be chased twice.

Where does CNC stop and inspection start?

Cutting stops at the last assembly surface; the inspection gate opens on the as-cast blank and closes on the finished part. The two are one chain rather than two departments.

Machining locates on the large-end flange face and on the bore axis, in a single setup. That datum holds the eight ⌀8.9 mm holes to a ⌀0.10 mm position and turns the ⌀61.5 +0.3/+0.1 spigot from the same axis.

The ⌀150 mm large-end flange arrives with 1.0 mm on its face and 0.4 mm in the holes. That stock lets the flange land at 0.05 mm flatness and Ra 3.2 µm roughness while the wall stays at 2.2 mm or more.

Roundness follows the same datum: 0.05 mm on the ⌀61.5 spigot and 0.02 mm in the ⌀24 boss bore. Both features are cut in the same clamping as the flange holes, so the axis does not have to be found a second time.

Tapping follows the cut, with G1/8 and M4 threads checked by go and no-go gauges. Nothing is polished to hide a casting defect; roughness is measured at three points per face and recorded against the part.

Inspection starts at the blank: radiographic testing (RT) to ASTM E192 level 2 and penetrant testing (PT) to ASTM E165 run before the first cut. After machining, a coordinate measuring machine (CMM) checks flatness, roundness, hole position and wall thickness on every part.

The cutting plan and the inspection points are written together inside the superalloy CNC machining route, and both appear on the same setup sheet. A dimension that no inspection step covers is caught on that sheet, before the cut rather than after it.

Two 3D scans bracket 1.0 mm of stock removal

Two 3D scans bracket the cut: the first records the blank, the second proves the part. Neither replaces the other, and a part released on one scan alone has an unproven half.

The first scan runs on the as-cast blank before any surface is cut. It reports deviation against the drawing plus 1.0 mm and is read as a map rather than a pass or fail. A blank that is short of stock on one side is straightened or re-datumed before cutting.

The second scan runs after machining and covers the full drawing, including faces a CMM stylus cannot reach. Both scans share a datum, so the difference between them is stock removal and not setup drift.

A scan report is judged on three fields: the datum it was aligned to, the allowance it was compared against, and the stated accuracy of the instrument. A number without those three is not a measurement of the part.

The method behind those numbers is set out in 3D scanning and measuring instrument checking, and the report follows the same fields. A scan taken with an unstated alignment cannot be compared with the next one.

Vacuum investment casting a combustor casing stops working below a 1.5 mm wall, past a flow length a 900 °C shell cannot carry, or where the drawing calls for directional or single-crystal grain. It also stops at an internal acceptance level tighter than ASTM E192 level 2; that is where hot isostatic pressing (HIP) enters the chain.

Send the wall thickness, the flange callout and the batch size, and Neway will return a route assessment with the stock, heat treatment and inspection points within two working days.


FAQs

  1. Can 2.5 mm Thin Walls Be Vacuum Cast in Hastelloy X?

  2. Which Datum Should a Vacuum Cast Casing Be Machined From?

  3. Is Hot Isostatic Pressing Required for Vacuum Cast Hastelloy X?

  4. What Flange Flatness Can a Vacuum Cast Casing Hold?

  5. What Lead Time Does a Vacuum Cast Casing Need From Wax?