What Flange Flatness Can a Vacuum Cast Casing Hold?

Table of Contents
Why does flatness move after solution treatment?
A 0.5 mm warp is cut back by 0.2 mm of stock
How is vacuum cast casing flange flatness released?
Above 0.15 mm, the flange goes to review

A vacuum cast casing flange holds 0.05 mm flatness after machining, and 0.30 mm while it is still in the heat-treated state. Solution treatment moves the flange about 0.5 mm, so a 0.2 mm correction pass is planned into the cut rather than discovered at inspection.

Why does flatness move after solution treatment?

The flange and the 2.5 mm cone cool at different rates. In a 1180 °C solution treatment with 2 bar argon cooling, the thick flange lags the thin cone, and the difference shows up as bow across the sealing face. Nothing is wrong with the furnace when this happens; it is the geometry.

Clamping during the cycle narrows the movement but does not remove it. A fixture that constrains the flange through the cool-down reduces the warp, and the part springs back a little when the clamps come off. The released value is what the machine shop receives.

Stress relief after shell removal is what keeps the movement predictable. Cleaning and cutting leave stress in the casting, and a 850 °C stress relief for 2 hours before the solution treatment gives a stable starting shape. Skipping it does not make the warp smaller; it makes it vary from part to part.

A 0.5 mm warp is cut back by 0.2 mm of stock

The correction is planned, not improvised. A 0.2 mm finishing allowance on the flange face covers the measured warp, and the first pass removes it in one clamping so the face is cut from a single setup. Cutting 0.2 mm in two setups reintroduces the error the allowance was meant to remove.

The rest of the 1.0 mm stock stays where it is needed. Wall thickness after cleanup has to stay at 2.2 mm or more, so the allowance is distributed between the face and the bore rather than taken entirely off the flange.

This is where the vacuum cast casing flange flatness target and the castability limit meet. If the as-cast warp exceeds what 0.2 mm can correct, the part is straightened before cutting and the measurement is repeated, rather than cut twice and hoped for.

How is vacuum cast casing flange flatness released?

Flatness is called out per ASME Y14.5 and measured on a coordinate measuring machine, on every part, with the datum stated on the report. A surface plate and a feeler gauge will find a 0.05 mm bow on a 150 mm flange only if the part is supported exactly as it will be bolted, which is why the CMM setup is written down.

CMM checking against a stated datum is what makes the number comparable between parts and between suppliers. A flatness figure without the support condition and the datum is not a release criterion for a vacuum cast casing flange, and the report is rejected on that basis.

The release point sits inside the wider superalloy CNC machining route, after stress relief and before the part is packed. Stress relief for dimensional stability is the step that makes the measurement repeat.

Stage

Value

Unit

Flatness after machining

0.05

mm

Flatness after heat treatment

0.30

mm

Warp after solution treatment

0.5

mm

Correction allowance

0.2

mm

Flange face stock

1.0

mm

Wall after cleanup

2.2

mm

Review threshold

0.15

mm

Above 0.15 mm, the flange goes to review

A flange that measures above 0.15 mm after machining is set aside for review instead of being pressed straight. Pressing a thin wall flat closes the gap on the plate and leaves elastic energy in the part, which returns as soon as the bolts are released.

The limit is not a tolerance on the drawing. It is the point where the remaining stock can no longer correct the face without taking the wall under 2.2 mm, so the decision moves from machining to a casting or heat-treatment fix.

Clamp force is the other trap. A casing that is clamped hard enough to remove 0.1 mm of bow will read flat on the machine and spring back 0.05 mm or more on the plate, which puts it back above the release limit.

Send the flange diameter, the flatness callout and the bolting condition, and we will state the correction allowance and the measurement setup before quoting the machining route.