English

Casting a Thin Wall Combustor Casing: Two Rework Loops

Table of Contents
What did the 193 mm casing have to hold?
The first cast failed ASTM E192 level 2 at mid-cone
Which changes closed the cold shut and shrinkage?
Solution treatment warped the flange 0.5 mm
What proves the casing is ready to ship?
FAQs

Thin wall combustor casing rework needed two loops: one for the cold shut, one for a 0.5 mm flange warp. The first loop changed the gating and added a 3 mm pad at the flange transition, which closed the mid-cone cold shut and the shrinkage behind it. The second loop changed how the flange was held through solution treatment and how much stock it carried into the cut.

Oblique view of a conical casing with two flanges and a side boss

Gloved hand holding a casing, spark plug boss on the conical wall

What did the 193 mm casing have to hold?

The 193 mm casing had to hold a 2.5 mm conical wall, an eight-hole ⌀150 flange and a ⌀24 boss seat on one axis. It sits around the combustor as a pressure shell, so the flange seals against the next casing at 0.05 mm flatness while the wall takes the pressure drop. No rib stands behind either feature.

The part is a 2.5 mm conical wall in Hastelloy X (UNS N06002), 193 mm tall, with a ⌀61.5 spigot at the small end and a ⌀24 boss on the cone for the igniter. Both ends thicken into flanges, and the cone between them has no stiffener, so the two frames carry the stiffness.

Release sits on three callouts: 0.05 mm flatness on the ⌀150 flange, 0.05 mm roundness on the ⌀61.5 spigot and ⌀0.10 mm position on the eight holes. The blank therefore carried 1.0 mm on the flange face and 0.4 mm in the eight holes for the cut.

The blank was scanned against the model before any cut, and that reading became the baseline the second scan later matched. Only the flange face, the eight holes and the boss seat were cut; the cone stayed as cast.

Two features are finished after the scan rather than cast: the boss seat and the eight flange holes. The threads are tapped last, after the assembly faces are cut.

The first cast failed ASTM E192 level 2 at mid-cone

The first cast of the thin wall combustor casing showed a cold shut across the mid-cone and shrinkage porosity in the flange-to-wall transition. Both came back on the first radiograph, before any heat treatment. The blank had already been scanned against the model, so each defect carried a location rather than a note.

The cold shut crossed the middle of the cone. The shrinkage sat where the 2.5 mm wall meets the ⌀150 flange. Neither defect touched the ⌀61.5 spigot or the boss seat.

Both were entered on the route log as feed gaps. That is what the first loop changed. The wall section was never on the list of changes.

The re-poured blank had to clear ASTM E192 level 2 by radiographic testing (RT) before the first loop could close. That gate is what separated the first loop from the second.

Which changes closed the cold shut and shrinkage?

Three changes closed both defects on the second pour of the thin wall combustor casing, and all three added feed rather than wall section. The first gave the mid-cone a second path, the second opened a channel into the transition, and the third kept that channel fed. The run was missing three things, and each one had a number attached.

  • Two in-gates on the mid-cone, so the front had a second and shorter path.

  • A 3 mm pad at the flange transition, so the thick section had a feed channel.

  • A riser 15 % larger and 60 min of in-mold cooling, so the transition stayed fed.

None of those changes touches the wall thickness. That is the point of the vacuum investment casting route: feed the blank, then let the cut bring it to size.

The shell was rebuilt around the same pattern and re-poured, so the wall section and the flanges did not change. Only the feed changed.

The re-shell kept the same five-layer build, and the pour ran at 1420 °C with the shell at 900 °C. Neither number moved from the first run.

Solution treatment warped the flange 0.5 mm

Solution treatment warped the flange 0.5 mm, and both casting defects were closed by then. The re-poured blank had cleared RT to ASTM E192 level 2, and solution treatment ran at 1180 °C for 1 h with a 2 bar argon cool. Stress relief followed at 850 °C for 2 h, the second half of the same superalloy heat treatment route.

The flange warp measured 0.5 mm across the ⌀150 flange (case file). A 2.5 mm wall and a flange that thick cool at different rates, so the thin side contracts first and pulls the face with it, which is the thin wall casting solidification rule behind the movement. The heat-treated band for the flange is 0.30 mm, and 0.5 mm sat outside it.

The second loop held the flange in the fixture through solution treatment and split the 2 bar cool into 1 bar for 30 s and then 2 bar. The flange was measured on a coordinate measuring machine (CMM) within 24 h of leaving the furnace, and the reading came inside the 0.30 mm band. The table below collects the five checkpoints that decided the release.

Checkpoint

First loop

Second loop

Unit

Record

Flatness after solution treatment

0.5

0.30 max

mm

CMM report

Correction cut, flange face

none

0.20

mm

Setup sheet

Flange flatness, machined

not reached

0.05

mm

CMM report

Flange review line

0.15

0.15

mm

Hold point

Loop time

5

4

working days

Route log

The correction cut took 0.2 mm off the flange face inside the 1.0 mm stock, and the 0.05 mm flatness target was met on the finished face. The flange face, the eight holes and the boss seat were cut in one computer numerical control (CNC) setup, with the flange face and the bore axis as one datum pair under ASME Y14.5. The superalloy CNC machining record from that setup is the release document.

The sequence below is the one that ran, and the one a second part would follow. Each step leaves a record behind it.

  1. Add two mid-cone in-gates, a 3 mm pad and a 15 % larger riser, then re-shell and re-pour.

  2. Radiograph the blank to ASTM E192 level 2 before any heat treatment.

  3. Constrain the flange in the fixture and run solution treatment with the split argon cool.

  4. Measure the flange on the CMM within 24 h of the furnace.

  5. Cut the 0.2 mm correction and the assembly faces in one setup, then run the second scan.

What proves the casing is ready to ship?

Three records prove the casing is ready to ship: the RT report to ASTM E192 level 2, the CMM report at 0.05 mm flatness and the second 3D scan against the baseline. The route did not use hot isostatic pressing (HIP).

The thin wall combustor casing rework took 9 working days, and the part still left on its original ship date. The first loop took 5 days: re-gate, re-shell, re-pour and radiograph. The second took 4 days: fixture, solution treatment, the 24 h hold and the correction cut.

The 9 days are the whole rework cost, not a per-loop average. Both loops were planned as route steps, not emergency work, so the schedule held. The stress relief in superalloy castings step is where that reservation is kept or lost.

What the record proves is narrow: the part was made to the drawing, inspected in house and released, and the two correction depths were measured. It does not prove customer acceptance, bench performance or third-party certification.

The route does not hold when the wall drops below 1.5 mm, when the flange warp runs past the 1.0 mm face stock, or when flatness at inspection is over 0.15 mm. Send the drawing, the wall section and the heat-treated flange reading, and Neway will reply within two working days with a route that carries both loops.


FAQs

  1. Can 2.5 mm Thin Walls Be Vacuum Cast in Hastelloy X?

  2. Which Datum Should a Vacuum Cast Casing Be Machined From?

  3. Is Hot Isostatic Pressing Required for Vacuum Cast Hastelloy X?

  4. What Flange Flatness Can a Vacuum Cast Casing Hold?

  5. What Lead Time Does a Vacuum Cast Casing Need From Wax?

================================================================================